Properties of our Manganese Zinc soft ferrite grades.

Parameter

Symbol

Standard Conditions of Test

Unit

F58

P11

P12

F5

F5A

F5C

F44

F44A

F47

F48

F63

F49

F9

F9C/F82

F10

FT7

F39

FTA

Initial

Permeability

(nominal)

µi

B<0.1mT

10kHz

250C

 

-

750

±20%

2250

±20%

2000

±20%

2000

±20%

2500

±20%

3000

±20%

1900

±20%

2400

±20%

1800

±20%

2300

±20%

3000

±25%

1000

±20%

4400

±20%

5000

±20%

6000

±20%

7500

±20%

10000

±30%

10000

±30%

Saturation

Flux Density

(typical)

Bsat

H=796A/m

=10 Oe

Static

250C

1000C

 

mT

450

-

-

-

-

-

470

350

470

350

460

330

500

400

510

-

470

350

480

380

500

400

580

460

380

-

460

-

380

-

420

-

380

-

420

-

Remanent

Flux Density

(typical)

Br

H→0 (from near Saturation)

10kHz

250C

 

mT

94

70

35

200

150

150

270

140

130

150

-

230

180

170

100

130

200

180

Coercivity

(typical)

Hc

H→0 (from near Saturation)

10kHz

250C

 

A/m

47

18

7

21

15

18

27

10

24

20

-

20

13

13

11

10

16

8

Loss Factor

(maximum)

tanδ/µi

B<0.1mT 10kHz

250C

100kHz

200kHz

500 kHz

1MHz

2 MHz

5 MHz

10 MHz

 

 

 

10-6

 

-

-

<12

-

<20

-

-

-

1.5

5

-

-

-

-

-

-

0.8

2.5

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

8

-

-

-

-

-

-

-

20

-

-

-

-

-

-

-

20

-

-

-

-

-

-

-

20

-

-

-

-

-

-

6

50

-

-

-

-

-

-

-

-

-

-

-

-

-

-

6

50

-

-

-

-

-

-

Temperature

Factor

αF

B<0.1mT

10kHz

+250C to 550C

10-6 /

0 C

 

0.5 –

2.3

0.5 –

1.5

0.4 –

1.0

-

-

-

-

-

-

-

-

-

0 to 2

-1 to 2

-1 to 2

-

-

-1 to 0

Curie

Temperature

(minimum)

θC

B<0.1mT 10kHz

0 C

200

150

150

200

200

180

230

210

200

220

230

290

130

160

130

150

120

150

Disaccomodation

Factor (max)

DF

B<0.1mT

500C

10 to 100 mins

10kHz

10-6

<12

4

3

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

Hysteresis

Material

Constant

(max)

ηB

B from1.5 to 3mT

10kHz

250C

10-6

mT

<1.8

0.8

0.45

-

-

-

-

-

-

-

-

-

1.1

-

-

-

-

-

Resistivity

(typical)

ρ

1V/cm

250C

Ohm-

cm

100

100

100

100

100

100

100

100

100

100

100

100

50

50

50

10

100

10

Amplitude

Permeability

(minimum)

µa

400mT 250C

320mT 1000C

340mT 1000C

-

-

-

-

-

-

-

-

-

-

2400

1825

-

2400

1825

-

2400

-

-

2500

-

1900

2500

-

-

2000

2500

-

2000

2500

-

2000

2500

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

Total Power

Loss Density

(maximum)

PV

200mT; 16kHz 250C

200mT; 16kHz 600C

200mT; 16kHz 1000C

200mT; 25kHz 250C

200mT; 25kHz 600C

200mT; 25kHz 1000C

200mT; 100kHz 1000C

100mT; 100kHz 250C

100mT; 100kHz 1000C

50mT; 400kHz 250C

50mT; 400kHz 1000C

mW/

cm3

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

120

110

110

-

190

190

-

-

-

-

-

120

110

110

-

190

190

-

-

-

-

-

120

120

110

-

190

210

-

-

-

-

-

-

-

-

200

-

130

750

250

160

-

-

-

-

-

-

-

-

380

-

80

-

-

-

-

-

120

-

100

-

110

80

150

150

-

-

-

-

-

-

380

-

70

-

-

-

-

-

150

-

120

340

-

120

-

170

-

-

-

-

200

-

1100

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-

-